How can the adhesion of silver paste and carbon paste for membrane switches be tested?
The adhesion test of silver paste and carbon paste for membrane switches is a crucial step in the quality control of membrane switches. There are several mature testing methods in the industry. The following will introduce them one by one according to their common usage:
3M Tape Method (The Most Common and Convenient)
This is the most widely used adhesion testing method in the membrane switch industry. It is simple to operate and the results are clear and intuitive.

Operation steps
1. Sample Preparation: After the silver paste/carbon paste is printed and fully cured, use a lint-free cloth dipped in isopropyl alcohol to clean the surface of the test area and let it dry.
2. Grid Treatment: Use a grid cutter (multi-edge cutter) to make a 10×10 grid on the coating surface, totaling 100 small squares. The spacing of the cutter is usually 1mm, and the cutting depth must penetrate the paste layer and reach the substrate.
3. Adhesive Tape Application: Use 3M 600 transparent tape (width 3/4 inch) to evenly stick on the grid area. Press firmly with fingers or an eraser to ensure that the tape is in full contact with the coating and there are no residual air bubbles.
4. Tape Removal: Wait for about 1 minute, then quickly peel off the tape in a 180° direction (speed approximately 300±100 mm/min).
5. Observation and judgment: Visually inspect the shedding of silver paste/carbon paste in the grid area.
Criteria for determination (ASTM D3359 / GB/T 9286)
| Grade | Area of peeling | Judgment |
| 0 grade | 0% (Edges are completely smooth, no peeling occurs in any area) | Best adhesion |
| Level 1 | ≤ 5% (only slight detachment at the crossing points) | Excellent |
| Level 2 | 5% - 15% | Good |
| Level 3 | 15% - 35% | General |
| Level 4 | 35% - 65% | Poor |
| Level 5 | > 65% | Poor |
In the membrane switch industry, a grade of 0 to 1 is generally required to be qualified. If the peeling area exceeds 5%, the adhesion is judged as unqualified.
Grid method (hundred-grid test)
Used in conjunction with the tape method, it focuses on directly observing the cohesive strength and adhesion state of the coating through grid cutting.
Tools: Special hundred-grid cutter (11 blades, spacing 1mm or 2mm)
Cutting requirements: Draw 11 vertical and 11 horizontal lines, forming 100 grids. The coating must be cut through to the substrate.
Cleaning: Use a soft-bristled brush to gently brush along the diagonal direction 5 times to remove loose particles.
Rating: Follow the 0-5 level standard of the tape method.
Pull-Off Test (Quantitative Test)
This method is used when specific adhesion strength values need to be obtained. It is applicable for research and development verification and critical product certification.
Principle: A standard-sized spindle (dolly) is adhered to the coating surface using a special adhesive. It is then pulled vertically with a tensile machine to measure the force required to detach the coating.
Standards: ASTM D4541, GB/T 5210
Result units: MPa or N/cm²
Advantages: Quantitative data, precise comparability
Disadvantages: Expensive equipment, complex operation, destructive test
This is a specific adhesion testing standard for membrane switches and printed electronic devices, which has been modified based on ASTM D3359.
Scope of application: Adhesion testing of inks and coatings with a thickness of ≤ 125 μm on flexible plastic substrates such as polyester (PET) and polycarbonate (PC)
Core method: Modified tape method, which solves the accuracy and repeatability issues of tape testing on plastic substrates
Limitations: Can only determine whether the adhesion meets an acceptable level, but cannot distinguish differences in higher levels of adhesion strength
GB/T 17473-2025 (The latest national standard)
The latest standard, which came into effect on May 1, 2026, integrates and replaces the original GB/T 17473.4-2008 adhesion testing method, and is applicable to precious metal pastes (including conductive silver pastes) used in microelectronics technology.
Differences in the tests of silver paste vs carbon paste
| Comparison items | Silver paste | Carbon paste |
| Test difficulty | Relatively easy (the silver layer is harder, making cutting clear) | Relatively difficult (the carbon layer is softer, prone to producing burrs) |
| Passing standard | Area of detachment ≤ 5% (0 - 1 level) | Area of detachment ≤ 5% (0 - 1 level) |
| Common Problems | Silver powder particles fall off, edges crack | Carbon layer flaking off, entire piece peeling off. |
| Supplementary tests | Sheet resistance test to verify conductive continuity | Abrasion test to verify surface hardness. |
Practical Operation Notes
Solidification Adequacy: Before testing, it is essential to ensure that the silver paste/carbon paste has fully solidified (typically at 120-150°C for 30-60 minutes). Samples that are not fully solidified have no reference value for the test results.
Environmental Conditions: The test should be conducted in a standard environment with a temperature of 23 ± 2°C and a humidity of 50 ± 5%. The samples must be left to stand in this environment for at least 16 hours.
Tool Condition: The cutting tool must be sharp. Using a blunt tool will result in uneven cutting edges, leading to incorrect judgments. It is recommended to check the cutting edge every 50 cuts.
Tape Consistency: The use of specified 3M tapes (600 or 810) is mandatory. The adhesion of different brands/models of tapes varies significantly and they must not be mixed.
Multiple Point Testing: At least 3 different positions of the same batch should be tested, and the worst result should be used as the judgment basis.
Double-Layer Structure Testing: For the double-layer structure of silver paste + carbon paste, the adhesion of the silver paste to the substrate (first test the adhesion of the carbon paste layer, then remove the carbon paste to test the silver paste layer) and the inter-layer adhesion of the carbon paste to the silver paste should be tested separately.
Summary: For daily production quality inspection, the 3M tape method combined with the grid marking method is recommended. This method is simple to operate, has low cost, and provides clear results. For research and development verification and for high-end product certification, quantitative testing using the pull-off method is suggested. The adhesion qualification standard for the film switch industry is usually a detachment area of ≤ 5% (0-1 grade). During the testing process, it is essential to ensure that the sample is fully cured, the environmental conditions are met, and the tools are standardized and consistent.