After the temperature resistance test is completed, one cannot simply rely on intuition for judgment. Instead, a strict quantitative assessment must be conducted based on the four dimensions of "appearance, function, structure, and physical properties".
Taking into account industry standards (such as GB/T 2423, IEC 60068) and the actual requirements of automotive/industrial-grade panels, I have compiled a detailed list of qualified judgment criteria for you:

Dimension 1: Visual Inspection (Most Intuitive)
This is the first step. It is usually conducted through visual inspection or microscopic observation 2 to 4 hours after the system has been restored at normal temperature.
| Inspection items | Passing criteria | Defective phenomena |
| Surface condition | Flat and smooth, without any changes | Bubble formation, delamination, warping, deformation (these are the most common failures) |
| Color/Glazing | Consistent with before testing, color difference ΔE < 1.0 | Yellowing, fading, darkening, or significant decrease in surface glossiness |
| Screen printing/characters | Clear and complete, sharp edges | Blurry, broken characters, ink peeling off, and jagged edges of the characters |
| Cracks | No cracks at all | Minor cracks (silver lines) at the edges or stress points |
Dimension 2: Electrical Function (Most Core)
Just because the appearance is fine doesn't mean the internal circuitry is intact. A multimeter or specialized testing fixtures must be used for inspection.
1、Loop Resistance:
Standard: Usually, it is required to be ≤ 100Ω (refer to the design drawings for specific values).
Judgment: The increase in resistance value after testing should not exceed 20%-30% of the initial value. If the resistance is infinitely large, it indicates that the circuit is broken (open circuit).
2、Insulation resistance:
Standard: Usually requires ≥ 100 MΩ (at 500V DC).
Judgment: Prevents short circuits between lines. Decrease in insulation performance after high temperature and high humidity is a common failure.
3、Key function:
Judgment: Each key must be able to trigger normally, without consecutive presses (pressing twice gives two characters), dead keys (no response after pressing), or accidental touches.
Dimension 3: Structure and Feel (Most Easily Ignored)
The structure specific to the film panel is evaluated.
1、Adhesion test (3M tape method):
Procedure: Draw a grid on the silk-screened or inked surface of the tested panel, then stick a 3M 600/610 tape on it and quickly pull it off.
Judgment: If the ink does not fall off, it is considered qualified (usually requiring a 5B grade). High temperatures often damage the adhesion between the ink and the substrate.
2. Button Feel (Force Test):
Operation: Use a push-pull force gauge to test the pressing force of the buttons.
Judgment: The feel force should be within the standard range (such as 170-397g). If the high temperature causes the silicone or spring clips to age, the feel will become soft (collapse) and unable to rebound.
3. Bulge/Window Deformation:
Judgment: The embossed areas should not have permanent collapse or irrecoverable deformation.
Dimension 4: Material Properties (Laboratory Level)
If conducting material validation (during the research and development stage), the following data also need to be considered:
Retention rate of tensile strength: The retention rate of the tensile strength of the material after testing should be ≥ 80%.
Break elongation rate: The material should not become brittle, and the retention rate of break elongation should be ≥ 70%.
Yellowing index: The change in the yellowing index of transparent PC/PET materials after high temperature should be within the allowable range.
Summary: Recommended Judgment Process
In actual operation, it is recommended to follow the following "three-step" process for judgment:
Hot-state observation (optional): If the operation can be performed in a high-temperature chamber, observe whether the panel has blistered or deformed under high temperature (many defects will recover after cooling, and hot-state observation is the most accurate).
Cold-state recovery: Remove and place it in standard atmospheric pressure (23°C, 50% RH) for 2-4 hours (some standards require 24 hours) to eliminate thermal stress.
Comprehensive inspection:
First, check: Are there any blisters or color changes?
Then, test: Are the on/off and resistance normal?
Finally, pull: Test the tape to see if the ink has peeled off?