How to adjust the process parameters when the thickness of the silver paste printing is uneven?
Uneven thickness of silver paste printing is one of the most common process defects in the production of membrane switches, directly affecting the consistency of contact resistance and the reliability of circuit conduction. The following is a systematic adjustment plan for process parameters:

Adjustment of screen plate parameters
The screen plate is the fundamental factor determining the thickness of the silver paste deposition. The following issues should be prioritized for investigation:
Screen mesh count selection: Conductive silver paste is recommended to use a mesh size of 200-250 (80-100 strands per centimeter), which can achieve a dry film thickness of 0.0005-0.0007 inches (approximately 12-18 μm). A too low mesh count will result in excessive film thickness and edge ink seepage; a too high mesh count will lead to insufficient ink penetration and higher resistance.
Uniformity of screen plate tension: Use a tension meter to measure at nine points on the screen plate, and the tension should be maintained at 18-25 N/cm, with the difference at each point controlled within ±1 N/cm. Inconsistent tension will cause differences in local ink penetration, resulting in thickness stripes. When the tension is lower than 85% of the initial value, the screen must be re-tensioned or replaced.
Thickness of photosensitive adhesive: Control the thickness of the adhesive layer through a capillary photosensitive film. The silver paste layer is recommended to use a photosensitive adhesive thickness of 40-50 μm, and the pattern layer uses 20-30 μm. Deviation in adhesive layer thickness will directly map to printing thickness deviation.
Screen distance (screen gap): The gap between the bottom of the screen plate and the substrate is recommended to be 1.0-2.5 mm. A too large gap will cause rapid rebound and trailing fringing; a too small gap will result in insufficient rebound and blurred patterns. The difference in gap at the four corners should be controlled within 0.5 mm.
Scraping tool parameter adjustment
The scraping tool is the most direct process method for adjusting the printing thickness. Four parameters need to be optimized in coordination:
Scraping knife hardness
It is recommended to use a hardness of 70-80 Shore A (medium soft). The higher the hardness, the cleaner the ink scraping and the thinner the film thickness; the lower the hardness, the greater the ink penetration, and the thicker the film thickness but with poorer uniformity.
Check the wear condition of the scraping knife edge after every 500 printing cycles. If there are notches or arc-shaped deformations, it must be ground or replaced in time; otherwise, it will cause uneven thickness in some areas.
Scraping knife angle
Recommended range: 60° - 75°. The smaller the angle (approaching 45°), the greater the ink deposition and the thicker the film; the larger the angle (approaching 80°), the less ink deposition and the thinner the film but with sharper edges.
Adjustment technique: First, fix other parameters and adjust the angle in increments of 5°. After printing a test strip, measure the film thickness using a thickness gauge and find the optimal angle for the target thickness.
Scraping pressure
Recommended range: 0.15 - 0.25 MPa (approximately 20 - 40 PSI). Excessive pressure will stretch the screen plate, causing pattern distortion and thinning of the film thickness; too little pressure will result in insufficient ink application and the appearance of pinholes and broken lines.
Pressure adjustment principle: Under the condition of ensuring complete ink application, use the minimum pressure.
Scraping pressure
The recommended range is 0.15 to 0.25 MPa (approximately 20 to 40 PSI). If the pressure is too high, it will stretch the screen plate, causing the pattern to deform and the film thickness to be too thin; if the pressure is too low, the ink will not be fully applied and pinholes and broken lines will occur.
Pressure adjustment principle: Under the condition of ensuring complete ink application, use the printing speed
The recommended range is 40 to 150 mm/s (approximately 6 to 12 inches/second). The slower the speed, the longer the silver paste stays under the scraping blade, and the thicker the film thickness; the faster the speed, the thinner the film thickness.
When the silver paste viscosity is high, the speed should not be too fast, otherwise, uneven ink application and line breaks are likely to occur. Minimum pressure.
Silver paste parameter adjustment
The rheological properties of the silver paste itself are the intrinsic determinants of uniform thickness:
Viscosity control: The optimal viscosity range for conductive silver paste is 25,000 to 40,000 cps. Excessive viscosity will cause difficulties in ink application and uneven thickness; too low viscosity is prone to ink leakage and blurred edges. The viscosity should be checked every 2 to 4 hours using a viscometer, with a temperature compensation of approximately 1,000 cps/℃.
Full stirring: The silver paste must be fully stirred for more than 20 minutes before use to prevent silver powder sedimentation, which can lead to local content differences and is a common cause of uneven thickness on the same printing plate.
Addition of diluent: If the viscosity needs to be adjusted, the addition amount of the diluent should be controlled within 5%. Excessive addition will reduce the solid content of the silver paste, resulting in insufficient film thickness and excessive resistance after curing.
Temperature management: The recommended usage temperature for the silver paste is around 25℃. Temperature fluctuations will cause changes in viscosity, thereby affecting the consistency of thickness.
Environmental parameter control
Temperature: The temperature in the printing workshop is controlled within 20-24℃ (with a fluctuation of ±2℃). If the temperature is too high, the solvent of the silver paste will evaporate faster and its viscosity will increase, resulting in a gradual decrease in the ink deposition amount.
Humidity: The relative humidity is controlled within 40%-60%. If the humidity is too high, the silver paste will absorb moisture and its rheological properties will change; if the humidity is too low, the solvent will evaporate too quickly.
Cleanliness: The workshop should reach at least ISO 8 level (100,000-level) cleanliness to prevent dust particles from adhering to the screen plate or the substrate, causing abnormal local thickness.
Thickness detection and feedback loop
Online film thickness measurement: Use a non-contact film thickness gauge (such as a laser thickness gauge) to measure in real time after printing. Take 5 to 10 samples from each batch, and the thickness deviation should be controlled within ±10%.
Resistance verification: After curing, measure the resistance using a four-probe resistance meter. If the resistance exceeds the standard ( > 50 mΩ/□), it usually indicates insufficient film thickness, and the printing parameters need to be retroactively adjusted in the opposite direction.
Weight monitoring method: Weigh the substrate before and after printing, calculate the amount of silver paste deposition based on the weight difference, and quickly determine whether the thickness is within the target range.
Order adjustment suggestions: When encountering uneven thickness issues, conduct a step-by-step investigation in the order of "screen plate tension → scraper parameters → silver paste viscosity → environmental conditions". In practice, approximately 60% of the uneven thickness problems stem from inconsistent screen plate tension or worn scraper edges. Prioritizing the inspection of these two factors usually enables quick identification of the root cause. During the adjustment process, only change one parameter at a time, record the data before and after the adjustment, and avoid changing multiple parameters simultaneously to prevent the inability to determine the cause-and-effect relationship.