How to conduct an oil resistance test for membrane keypads?
The oil resistance test for the membrane keypads is mainly to evaluate the anti-permeation and anti-pollution capabilities of the surface materials (such as PET or PC films) towards oily substances. In the industrial and material testing fields, quantitative analysis is usually conducted based on standardized testing methods. Here are several mainstream oil resistance testing methods and related standards:

I. Standard Oil Resistance Testing Method (Applicable for Laboratory and Factory Inspection)
1. KIT Oil Resistance Grade Test (ISO 16532-1)
This is a quantitative analysis method commonly used to evaluate the oil resistance performance of films, coatings, or papers.
Test Principle: Twelve different surface tension mixed solutions (prepared by blending castor oil, toluene, and n-heptane in different proportions, with the first one being the most oily and the twelfth one the most water-based) are used to simulate oils.
Operation Procedure: Place the sample to be tested flat as a membrane keypad sample, and drop the above solutions onto the coated surface. Let it stand for 15 seconds.
Result Evaluation: Observe which solution first leaves a stain or penetrates on the film surface. The grade corresponding to that solution determines the oil resistance grade of the film. The higher the grade, the better the oil resistance performance.
2. Oil Resistance Grade Test (GB/T 19977 / ISO 14419 / AATCC 118)
This series of standards is mainly used to evaluate the material's ability to resist the absorption of different surface tension liquid hydrocarbons.
Test principle: A series of standard hydrocarbons with decreasing surface tension (such as mineral oil, n-hexadecane, n-heptane, etc., totaling 8 grades) are used.
Operation procedure: Place the film sample face-up on a white absorbent pad. Use a dropper to carefully drip 5 drops (with a diameter of approximately 0.5mm) of the test liquid at a height of about 6mm from the sample surface, with an interval of approximately 4.0cm between the drops.
Result evaluation: Observe the state of the liquid droplets at a 45° angle within 30 seconds. The higher the oil resistance grade, the better the sample's ability to resist oil contamination.
II. Special Technical Condition Testing for membrane keypads
If the target is a finished membrane keypadboard, the test of chemical resistance performance as stipulated in the national standard GB/T 30091-2013 "Technical Conditions for membrane keypadboards" can also be referred to:
Test purpose: To verify the keyboard surface and keys' tolerance to chemicals that may be encountered daily (including cleaners, hand oils, solvents, etc.).
Test method: Use the specified chemicals or oils to wipe or come into contact with the keyboard surface, and observe whether there are phenomena such as corrosion, swelling, delamination or performance decline on the film surface.
III. Collaborative Protection Measures for Daily Oil Prevention
In addition to the rigorous tests conducted before shipment, the oil prevention effect of the membrane keypads during actual use is also closely related to daily maintenance. To extend the lifespan of the membrane keypads and maintain the feel, the following protection strategies are recommended:
Physical Isolation: Select a keyboard film with a thickness of approximately 0.25mm and a transmittance of over 92%, made of TPU material. This can effectively prevent hand oil from reaching the keycap body, significantly reducing the probability of contact with oil.
Scientific Cleaning: If the surface is stained with oil, use 75% - 99% concentration isopropyl alcohol (or anhydrous ethanol) in combination with dust-free cotton swabs for meticulous wiping. Isopropyl alcohol evaporates quickly and leaves no residue, and it can efficiently dissolve oil without damaging the coating on the film surface. For stubborn oil films, an electronic-grade cleaning paste can also be used for adsorption treatment.