    How to conduct the hand-sweat resistance test for membrane keypads?

    2026-06-17

    The hand-sweat resistance test of the membrane keypads is an important part for evaluating their reliability, corrosion resistance and appearance retention under long-term exposure to human sweat. The standard hand-sweat resistance test usually consists of three core steps: the preparation of artificial sweat, the execution of the test method, and the final performance evaluation.

    productive process (19).jpg

    I. Test Medium: Preparation of Artificial Sweat
    Since direct collection of human sweat is not feasible, in the tests, "artificial sweat" prepared by chemical means is usually used for simulation. According to industry standards (such as QB/T1901.2-93), the common formulas and preparation methods for artificial sweat are as follows:
    Chemical Components: Sodium Chloride (NaCl) 20g/L, Ammonium Chloride (NH₄Cl) 17.5g/L, Urea (CH₄N₂O) 5g/L, Acetic Acid (CH₃COOH) 2.5g/L, Lactic Acid (C₃H₆O₃) 15g/L.
    pH Adjustment: Sodium Hydroxide (NaOH) is used to adjust the pH value of the solution to 4.7.

    II. Standard Testing Methods
    For the characteristics of membrane keypads, the hand-sweat resistance test mainly adopts the following three methods:
    1. Sweat Streak Friction Test (Most commonly used)
    This method simulates the process of human hand touching and repeated friction, and comprehensively assesses the durability of the product by combining the corrosive effect of sweat.
    Operation: Use a professional fingertip wear resistance tester or friction tester, apply the specified load (usually between 1N and 100N) on a 10mm or 20mm silicone fingertip test head. Set the friction stroke (1mm to 4mm) and the number of cycles. Perform back-and-forth friction on the keypad surface in dry grinding or chemical-mechanical combined wear mode.
    2. Immersion Test
    Operation: Hang or fully immerse the membrane keypad sample in a constant temperature (usually 40 ± 2℃) artificial sweat container, and expose it for at least 24 hours to evaluate its corrosion resistance and anti-peeling layer ability in the sweat environment.
    3. Drip Test
    Operation: Drop a quantitative amount of simulated sweat on the surface of the membrane keypad, maintain it under specific temperature and humidity conditions for a specified period of time, and observe the corrosion and adhesion effects of the sweat on the local area.

    III. Evaluation Criteria after Testing
    After the testing is completed, the membrane keypads need to be comprehensively evaluated from three aspects: appearance, functionality, and electrical performance:
    Appearance and adhesion assessment: Check if there are any corrosion phenomena such as color change, loss of luster, blistering, or peeling on the keypad surface. For character adhesion, confirm that the printed characters do not wear off or fall off under the influence of sweat and friction (for example, if the corrosion area is no more than 1.5 square millimeters, it is considered qualified).
    Mechanical and operational performance: Confirm whether the key can function normally, and whether it still has good elasticity when pressed and released, without sticking or malfunctioning. The variation range of pressing force and rebound force should generally be controlled within ±15%.
    Electrical reliability: Use professional instruments to measure the change rate of the contact resistance of the key. If the resistance change exceeds 20% or there is a short circuit phenomenon, it is considered failed. At the same time, it is necessary to ensure that the insulation resistance (at 100V DC ≥ 100 megohms) meets the standard to prevent internal circuit leakage or short circuit due to sweat infiltration.