How to repair the oxidation of the thin film circuit?
Film circuit oxidation is a common cause of button malfunction. Due to the fragile nature of the conductive layer in membrane switches (usually silver paste or carbon powder), when repairing, the principle of "gentle cleaning first, then precise re-wiring" must be followed. Here is the standard repair process:

1. Gentle Physical and Chemical Cleaning (Preferred Option)
For mild oxidation, usually no additional wire bonding is required. The conductivity can be restored by removing the oxidized layer.
Physical polishing: Take a clean drawing eraser and wipe the oxidized and darkened copper contacts at a 45-degree angle in one direction for 3 to 5 times until the contact surface regains a mirror-like metallic luster. This method can effectively reduce the contact resistance to below 50Ω.
Chemical cleaning: Use a lint-free cloth or cotton swab dipped in 99% pure isopropyl alcohol (isopropanol) to gently wipe the contacts and the surrounding areas, removing grease and stubborn oxide residues. After it naturally evaporates and dries, testing can be conducted.
2. Precise repair with conductive silver paint (for broken circuits or severe oxidation)
If the device still fails to function after cleaning, or if a multimeter detects micro-cracks or open circuits in the circuit, conductive silver paint should be used for repair.
Expose the base layer: Use 300-mesh sandpaper or a utility knife tip to gently scrape off about 0.5 to 2 millimeters of the insulation layer at both ends of the break or severely oxidized area. Be very careful to expose the underlying copper foil and never scratch through the base film.
Apply silver paint: Mix the conductive silver paint pen well, and draw a continuous silver line in a single-direction dragging motion between the scraped-off copper foil in a slightly wider shape than the original circuit (the coverage length must extend more than 1.2 millimeters on both sides of the break). It is recommended to apply in 2-3 thin layers, with an interval of 30 seconds to 1 minute each time.
Allow to stand and cure: After coating, place it flat and let it dry for 4-5 minutes or more. During this period, do not touch the un-dried silver line. Wait until it is fully cured before conducting an electrical test.
3. Elastic Conductive Silicone Repair (for detached or cracked contacts)
If the conductive carbon or silver dots on the film have fallen off or flaked off, you can use a special elastic conductive silicone (such as nickel-carbon conductive silicone).
Procedure: Apply a small amount of the conductive silicone to the edge of the detached contact and gently press it down. This adhesive is elastic and resistant to bending, and after drying, it not only restores conductivity but also retains the spring-back feel of pressing, unlike ordinary 502 glue which becomes hard and insulating.
Repair Precautions:
Ordinary solder must not be used: The PET substrate of the membrane switch is extremely heat-resistant. Using an electric soldering iron will instantly burn through the film, leading to complete scrapping.
Evaluate repair value: If the film shows extensive wear, the PET substrate turns yellow and brittle, or the printed circuit lines are broken in multiple places, it indicates that the film has undergone irreversible fatigue aging. At this point, DIY repair is difficult to ensure long-term stability. It is recommended to directly replace with a brand-new film component of the same model.