How to solve the problem of insufficient adhesion of silver paste circuits?
The insufficient adhesion of silver paste circuits is one of the most common quality problems in the production of membrane switches, which can lead to circuit detachment, short circuits and even product failure. To solve this problem, a systematic investigation needs to be conducted from four aspects: substrate treatment, material matching, curing process and printing control.

Surface treatment of the substrate (the most common cause)
The surface energy of PET and other film substrates is low and they have strong chemical inertness, which is the primary reason for poor adhesion.
Corona treatment
Target value: The surface tension of the substrate must be ≥ 38 dyne/cm (dyne units), with the ideal range being 40 to 42 dyne/cm.
Testing method: Use a dynometer pen to draw lines on the substrate surface. Continuous lines indicate compliance, while intermittent lines indicate insufficient treatment.
Time requirement: Printing must be completed within 24 to 48 hours after corona treatment. If the time limit is exceeded, the surface energy will decrease, and re-treatment will be necessary.
Plasma treatment (advanced method)
For products with extremely high adhesion requirements (such as automotive and medical products), plasma treatment equipment can be used. It can increase the surface energy of PET from 38 dyn/cm to above 52 dyn/cm within a short period of time, and the effect is superior to corona treatment.
Cleaning and Decontamination
The release agent on the substrate surface, fingerprints and dust are all factors that reduce adhesion. Before printing, the substrate must be wiped with anhydrous alcohol. The operator should wear anti-contamination gloves throughout the process.
Material Matching and Selection
The compatibility between the silver paste and the substrate
Different substrates (PET, PC, PI) require the use of corresponding special silver pastes. For example, for PET substrates, the model with optimized adhesion should be selected, and for PI substrates, the model resistant to high temperature and bending should be chosen.
If it is confirmed that the materials do not match, the corresponding substrate-specific pastes must be replaced.
Selection of insulating ink
The silver paste lines of the membrane switch are sandwiched between the PET substrate and the insulating ink layer. When the insulating ink solidifies, the internal stress generated will compress the silver paste lines, resulting in reduced adhesion and even breakage of the silver layer.
It is recommended to use an insulating ink with good compatibility with the silver paste (such as Acheson Electroday 452SS), and adopt a semi-circular printing mode for the insulating layer to reduce the pressure on the silver paste lines.
Solidification process control (key factors)
Insufficient curing is the second major cause of poor adhesion. The resin in the silver paste needs to undergo complete cross-linking and curing in order to form a strong bond with the substrate.
Recommended curing curve
After the silver paste is printed, it cannot be directly subjected to high-temperature baking. Instead, a staged heating process for curing should be adopted:
Pre-drying: 80~100℃ × 30 seconds (infrared low-temperature drying), allowing the solvent to slowly evaporate from the bottom
Medium-temperature curing: 120~130℃ × 2~3 minutes (or 130℃ × 40~60 minutes)
Final curing: 150℃ × 30 minutes (convection oven), ensuring complete cross-linking of the resin
The dangers of insufficient solidification
Insufficient temperature or time can result in incomplete resin cross-linking, significant reduction in adhesion, and an increase in resistance.
A sudden temperature rise (for example, from room temperature to 120℃) can cause the substrate to deform or the silver paste to crack. It is necessary to increase the temperature slowly.
Cooling after solidification
After the curing process is completed, it should naturally cool to room temperature. Avoid forced cooling as it may cause the substrate to contract or the silver paste to crack.
Control of printing process parameters
Pre-treatment of silver paste before use
Thorough stirring: Before use, it must be stirred for more than 20 minutes to re-distribute the settled silver powder evenly.
Temperature recovery: The silver paste stored in the refrigerator needs to be taken out 4 hours in advance and restored to room temperature before stirring and use.
Avoid adding solvents randomly: Adding solvents will disrupt the solid content ratio of the silver paste, affecting adhesion and conductivity. If dilution is necessary, it should be done by precisely weighing and adding.
Film thickness control
If the silver film thickness is insufficient (less than 8 μm), the adhesion will decrease. It is recommended to use a 80-100 T/cm (approximately 200-250 mesh) screen for printing, and monitor the film thickness through the resistance value.
If the film thickness is too thick, the solvent will not evaporate sufficiently during curing, which will also affect the adhesion.
Screen plate and scraper
Insufficient net plate tension can lead to uneven printing pressure and insufficient local film thickness. The tension should be controlled within 18 to 25 N/cm.
Scraping knife wear can cause printing defects. It is recommended to inspect once every 500 prints.
Adhesion test method
After the problem is solved, it must be verified through standard tests:
Berg Test (ASTM F1842): Draw 10×10 1mm squares, apply 3M 600 tape, then peel it off. The area of detachment should be ≤ 5% (4B grade) for qualification.
Bending Test: After bending repeatedly 5 to 10 times, the increase in resistance should be ≤ 30% for qualification.
Tensile Test: Quantitatively measure the peel strength using a tensile testing machine.
Quick troubleshooting flowchart
Poor adhesion → Step 1: Use a DynaPen to test the surface tension of the substrate
├─ < 38 dynes/cm → Add additional curing haze / perform plasma treatment
└─ ≥ 38 dynes/cm → Step 2: Check the curing process
├─ Insufficient temperature/time → Strictly follow the segmented curing curve
└─ Normal curing → Step 3: Check material compatibility
├─ Silver paste does not match the substrate → Replace with a dedicated silver paste
└─ Matched → Step 4: Check printing process
├─ Insufficient film thickness → Adjust the mesh count of the screen or the thickness of the photosensitive胶
└─ Normal film thickness → Check the insulating ink mode (change to semi-circular mode)
💡 Summary: The core solution approach for insufficient adhesion of silver paste is to first treat the substrate surface (electrostatic treatment ≥ 38 dynes/cm), then ensure complete curing (segmented heating, 130-150°C), then verify material compatibility (matching between silver paste and substrate), and finally control printing parameters (film thickness above 8 μm, screen size 80-100 T/cm). In actual production, more than 80% of adhesion issues occur in these two aspects: substrate surface treatment and curing process. It is recommended to prioritize the investigation of these two aspects.