    Featured News

    What should be noted when printing the conductive carbon paste for membrane switches?

    2026-05-22

    Conductive carbon paste printing is a key process in the production of membrane switches, directly affecting the on-resistance, feel and long-term reliability of the keys. The following are several aspects that require special attention:

    machinery equipment (2).jpg
    1. Environmental control: Temperature and humidity are the silent killers
    Temperature: The optimal printing environment temperature is 20-25℃. If the temperature is too high, the viscosity of the carbon paste will decrease, resulting in a thinner printing thickness and line diffusion; if the temperature is too low, the fluidity of the carbon paste will deteriorate, making it prone to clogging the screen.
    Humidity: This is the most critical issue to be vigilant about in Dongguan at this time. The relative humidity should be controlled at 40-60%. If the humidity is too high (>70%), the carbon paste will absorb moisture from the air, leading to:
    Conductive performance degradation: The moisture will hinder the contact between carbon particles, causing an increase in the sheet resistance value.
    Adhesion deterioration: Moisture remaining between the carbon layer and the PET substrate causes subsequent carbon layer detachment.
    Bubbling/holes: After drying after printing, the evaporation of moisture will form bubbles or holes.
    Cleanliness: It is recommended that the printing workshop reach a 100,000-level clean standard. Dust, fibers, and other impurities falling into the carbon paste will cause short circuits or breaks in the circuit.

    2. Ink Preparation: Stirring and Viscosity
    Full Stirring: The carbon powder and resin in the carbon paste are prone to settle. Before use, it must be stirred with a mixer at a speed of 300-500 rpm for 10-15 minutes until the ink is completely uniform and without any layering. Be careful not to generate air bubbles during stirring.
    Viscosity Control: The viscosity of the carbon paste usually ranges from 5000 to 25000 mPa·s (depending on the brand and model). During printing, the viscosity should be maintained within the range of 8000-12000 mPa·s. Excessive viscosity can cause stringing and mesh blockage during printing; too low viscosity will result in diffusion of lines and insufficient thickness.
    Ready-to-use: The prepared carbon paste should be used up within 4 hours. Any unused ink should be sealed and re-stirred before the next use.

    3. Screen Selection: Precision and Thickness
    Screen mesh size: It is recommended to use polyester screens with a mesh size of 250-300 or stainless steel screens with a mesh size of 200-250. If the mesh size is too low, the carbon paste deposition will be too thick, and the edge of the lines will be blurred; if the mesh size is too high, the carbon paste will be difficult to pass through, resulting in insufficient thickness and poor conductivity.
    Photographic film thickness: It is recommended to control the thickness within 10-15 μm. If the photographic film is too thin, the carbon paste film will be insufficiently thick; if it is too thick, the line precision will decrease.
    Tension control: The screen tension should be maintained at 22-28 N/cm. If the tension is insufficient, the screen will deform during printing, leading to deviations in line dimensions.

    4. Printing Parameters: Pressure, Speed and Angle
    Scraping Knife Hardness: It is recommended to use a polyurethane scraping knife with a hardness of 70-80 degrees. If it is too hard, the screen plate will be easily worn; if it is too soft, the ink transfer will not be uniform.
    Scraping Knife Angle: The scraping angle should be controlled at 60-75 degrees. If the angle is too large, the ink is scraped too clean, resulting in insufficient deposition; if the angle is too small, there is too much ink residue, and the lines become blurry.
    Printing Pressure: The pressure should be adjusted to just ensure that the carbon ink is completely transferred to the substrate, usually at 3-5 kg/cm². If the pressure is too high, the screen plate will deform, and the lines will become thicker; if the pressure is too low, the carbon ink transfer will not be complete, and there will be broken lines.
    Printing Speed: It is recommended to control at 200-400 mm/s. If the speed is too fast, the ink cannot be transferred in time, resulting in insufficient thickness; if the speed is too slow, the production efficiency will be low, and the ink is prone to drying on the screen plate.

    5. Drying and Curing: Determining Final Performance
    Drying method: It is recommended to use a combination of infrared pre-heating and hot air circulation.
    Infrared pre-heating: Preheat at 80-100°C for 30-60 seconds to quickly evaporate the solvent and prevent bubbling.
    Hot air curing: Cure at 135-150°C for 25-35 minutes to allow the resin to fully crosslink and ensure that the carbon particles are closely attached.
    Curing degree determination: For a fully cured carbon film, conduct a vertical pull test with 3M 600 adhesive tape. There should be no carbon powder shedding. The sheet resistance value should reach the technical specifications provided by the supplier (usually 200-250 Ω/□ or lower).
    Note: Insufficient curing results in high carbon film resistance and poor adhesion; excessive curing causes the carbon film to become brittle and prone to cracking.

    6. Common Defects and Countermeasures

    Defect Possible Causes Countermeasures
    Jagged edges of lines Too low mesh count of the screen, insufficient thickness of the photosensitive gel, worn-out scraper Increase mesh count of the screen, increase thickness of the photosensitive gel, replace the scraper
    Uneven carbon film thickness Unequal scraper pressure, inconsistent screen tension, change in ink viscosity Adjust scraper pressure, check screen tension, control ink viscosity
    High resistance value Too thin carbon film, insufficient curing, expired or improperly mixed carbon paste Increase printing thickness, extend curing time, replace or re-mix the carbon paste
    Poor adhesion Insufficient surface activity of PET substrate, mismatch between carbon paste and substrate, insufficient curing Use a dynometer to test the surface tension of the substrate (must be > 38 dyn/cm), replace the carbon paste, enhance curing
    Pinholes/Bubbles There are air bubbles in the ink, printing speed is too fast, drying temperature rises too quickly Decompress by stirring after mixing, reduce printing speed, adopt stepwise temperature drying
    Short circuit/Disconnection Defects in the screen, dust entering during printing, too small line spacing Inspect the screen, improve workshop cleanliness, optimize circuit design

    Summary: The core of conductive carbon paste printing lies in "controlling the environment, adjusting the viscosity, selecting the screen, setting parameters, and ensuring curing". As long as these key points are well grasped, high-quality film switches can be reliably produced.