Welcome to LuphiTouch®!
Today is 2026.11.05 , Thursday
Leave Your Message
News Categories
    Featured News

    Will a too-thin silver coating layer cause poor contact?

    2026-06-22

    A too thin silver paste film layer does indeed lead to poor contact, and this is an important root cause of membrane switch failure. The following is a detailed mechanism analysis and corresponding suggestions: 

    productive process (14).jpg
    Film thickness standard reference

    The industry standard for the dry film thickness of conductive silver paste for membrane switches is 7 to 12 μm. The sheet resistance should be less than 50 mΩ/square, and the resistivity should be lower than 0.5 Ω·cm. If it falls below this range, both electrical performance and reliability will significantly deteriorate.

    The mechanism of poor contact due to too thin film thickness 

    Excessive contact resistance

    The thickness of the silver paste directly determines the cross-sectional area and conductivity of the circuit. When the paste thickness is insufficient, the conductive path becomes narrower, causing the contact resistance to soar from the normal value of <3Ω to tens or even hundreds of ohms, resulting in unstable signal transmission and manifested as sluggish button response or intermittent failure.

    The underlying substrate is exposed after the silver layer wears off.

    This is the most critical failure mechanism. During the use of the membrane switch, the contacts undergo tens of thousands of pressing and frictional actions. When the film thickness is sufficient, the silver layer can withstand long-term wear; but when the film thickness is too thin, the silver layer will be worn through after tens of thousands of presses, exposing the underlying copper substrate. Copper's anti-oxidation ability is much weaker than that of silver. Once exposed, it rapidly oxidizes to form a high-resistance oxide film, causing the contact resistance to sharply increase, and eventually resulting in a complete circuit break.

    Micro-battery effect accelerates corrosion

    When the silver layer is locally too thin or there are pinholes, a micro-battery will form between the silver and the copper substrate in a humid environment, accelerating the electrochemical corrosion of the copper substrate and further deteriorating the contact performance.

    The risk of line breakage increases.

    Insufficient film thickness will also reduce the mechanical strength of the silver paste lines. Under stress such as bending and thermal expansion and contraction, micro-cracks are more likely to occur and even lead to line breakage, resulting in circuit failure.

    Characteristics of insufficient film thickness

    • Initial stage: Contact resistance is relatively high but still conductive. Button response is occasionally delayed.
    • Mid-stage: Resistance continues to increase. Greater force is required to trigger the button.
    • Late stage: Silver layer is worn through, and copper substrate is oxidized. The button completely fails to function.

    Preventive and improvement measures

    Process end

    • Increase printing frequency: When the single printing film thickness is insufficient, a two-printing method with layering can be used to reach the target thickness (0.0005 - 0.0007 inches), but it is necessary to ensure that the first layer is fully cured before printing the second layer.
    • Adjust scraper parameters: Reducing the hardness of the scraper (70 - 75 Shore), decreasing the angle (15° - 25°), and lowering the printing speed (4 - 8 inches per second) can all increase the ink deposition.
    • Select high-solid content silver paste: Silver paste with a solid content of 65% - 75% can achieve a larger dry film thickness under the same printing conditions.

    Testing end

    • Online film thickness monitoring: Use a non-contact film thickness meter to measure in real time, with the deviation controlled within ±10%
    • Resistance inspection: Measure the resistance after curing using the four-probe method. If the resistance exceeds ( > 50 mΩ/□ ) it indicates insufficient film thickness
    • 3M tape test: Verify the adhesion of the silver paste, preventing local detachment due to uneven film thickness

    Design end

    1. Thickening of key contact areas: Perform local secondary printing and thickening treatment on the contact area to increase the wear resistance margin
    2. Carbon layer coverage protection: Print a layer of carbon paste on the surface of the silver paste circuit as a protective layer, which not only prevents oxidation but also enhances wear resistance
    3. Summary: If the thickness of the silver paste film is too thin, it not only leads to a high initial contact resistance, but also significantly shortens the lifespan of the switch - after the silver layer is worn through, the copper substrate rapidly oxidizes, and the poor contact will irreversibly deteriorate. It is recommended to control the film thickness within the standard range of 7 to 12 μm, and verify the conductive performance and adhesion through both sheet resistance testing and 3M tape testing to ensure that both the conductive performance and adhesion meet the requirements simultaneously.